用溶胶-凝胶(Sol-Gel)法制备了RE(RE=La,Y)-Mo复合氧化物粉末,工艺条件:初始溶液pH值=1,于550℃分解胶体,500℃,900℃2次还原粉末.采用XRD,TEM对还原后粉末的相组成、形貌、粒度进行分析.结果表明:500℃还原后,单质Mo衍射峰出现,RE以非晶态RE-O-Mo存在;900℃2次还原后,RE以氧化物形式存在.红外光谱(FT-IR)分析结果表明,La和Y通过O与Mo键合,削弱Mo=O键,使稀土钼复合氧化物可还原性增强.TEM分析表明,还原后稀土钼粉末粒径在70 nm左右.